| STANDARD OPERATING PROCEDURE | |
| CORAL Name: | sts3 |
| Model Number: | ST Systems Multiplex ICP |
| Location: | TRL |
| What it does: | deep silicon etch system |
| Introduction: | The ST Systems Multiplex ICP tool is a Deep Reactive Ion Etch (DRIE) system. It provides high aspect ratio etching and deep/through wafer anisotropic etching capabilities. The tool uses two independent 13.56MHz Radio Frequency (RF) power supplies - a 1000W supply for a single-turn coil around the etch chamber and a 300W supply connected to the wafer electrode - to vary the RF bias potential of the wafer with respect to the plasma. The efficient inductive power coupling of the coil to the plasma allows high density plasmas to be maintained. The tool uses the Bosch process of time multiplexed deep etching (TMDE) to achieve high aspect ratio etches. This process utilises an etch cycle flowing only SF6 and then switching to a sidewall passivation cycle using only C4F8. During the subsequent etch cycle, the passivating film is preferentially removed from the bottom of the trenches using ion bombardment. |
| Safety: | Due to the toxic nature of the process gases, the supply cylinders are turned on and off by qualified technical staff only. All tank changes are performed by qualified technical staff only. Do not try to defeat any interlock on the system. Keep your hands away from all moving parts and be sure that all covers are in place when you are processing. If you encounter any equipment problems while operating the system, contact the technical staff in charge of the system. Do not try repairs on your own. |
| Procedure: | It is mandatory to reserve the system prior to use and to ENGAGE MACHINE prior to starting your process in CORAL. Loading a Wafer: The wafer is loaded using the Wafer Transfer Window located on the lower right of the screen:
Vent the loadlock by clicking on the Vent button:
Manually load the wafer onto the load arm using a pair of tweezers and click the Pump + Map button. Using a Sequence: Load the desired sequence using the Sequencer window located on the middle right side of the screen:
Click on the Open button to display the list of available sequences. Use the View button to check that the selected sequence utilises the correct recipe and the Batch number is correct for your number of wafers.
Before beginning the process, open the Recipe Editor and ensure that the correct process time has been entered (see the Editing a Recipe section below). If everything is correct, click on the Run button on the Sequencer window. The system will automatically load the wafer, run the recipe and unload the wafer to the loadlock. When the wafers have completed processing, they will turn green and can be removed from the loadlock by clicking the Vent button on the Transfer window. Using Manual Mode: After clicking the Pump + Map button, the wafer loaded will appear in the Plan View window. The wafer is loaded into the process chamber by clicking on the Load button on the Transfer window. When the wafer has been loaded, the desired process can be selected by clicking on the Select button on the lower left of the Process Control window.
Once the recipe has been loaded, click on the Process button to begin running the process. When the recipe has completed, click on the Unload button on the Transfer window to remove the wafer from the chamber, click on the Vent button to vent the loadlock and remove the wafer.
Recipe Editing: To open the Recipe Editor, click on the Recipe button on the bottom centre of the Process Control screen.
On the General control screen the process time may be adjusted – the process length can be set by time or by number of etch/passivation cycles. This step allows to you change the ProcessTime. The Pressure, Gases, R.F.,HBC and HeLUR tabs may be clicked on to view the recipe parameters but no other set point should be adjusted without consulting the Engineer in charge of the tool. If there are any issues with the tool post a comment in CORAL and contact Donal 2-2983. |
| Author: | Donal Jamieson, 12/05 |
"...A broad array of technologies that can be employed across an enormous breadth of investigation..."