Using MTL » Fabrication » Standard Operating Procedures

tube6A-npoly

STANDARD OPERATING PROCEDURE
This equipment donated by Intel
CORAL Name: tube6a-npoly
Model Number: Thermco LPCVD polysilicon reactor
Location: ICL
What it does: Low-pressure chemical vapor deposition reactor.
Introduction:

THERMCO “6A-nPoly” Furnace is a Low Pressure Chemical Vapor Deposition (LPCVD)Reactor, designated to deposit Phosphor Doped PolySilicon thin films on Silicon wafers up 6 inch in diameter. The Polysilicon film is deposited by pyrolysis of Silane (SiH4)  and Phosphine (PH3) at low pressure( 150 – 300 mTorr) in the temperature range of 560 – 625° C.

The process runs in the “Reaction Rate Limited Regime”; i.e. operating at low pressure the mean free path of the reactant gases is high and assures an uniform gas supply, so the mass transfer to the Silicon substrate does not limit the deposition rate. In this regime the deposition thickness is a linear function of time.

The Silane and the 1.5%PH3/SiH4 mixture are injected into the reactor at the Load zone, and the vacuum port is located at Source zone end.
The temperature profile is tilted, with a higher value at the Source end to compensate the Silane depletion due to the vacuum pump action. The system low pressure is maintained by thortle valve control at constant gas flow.

The Polysilicon deposition process parameters are:

  • Temperature : 560 -625 °C
  • Pressure: 200 mTorr
  • SiH4 flow: 150 sccm
  • 1.5%PH3/SiH4 flow: 40sccm
  • deposition rate is constant: 30 A/ min
  • Thickness uniformity across the wafer : < 1.5 % @ 2,500 A
  • electrical resistivity : < 0.003 Ohm-cm

The THERMCO furnace is controlled by the TMX tube computer; while the SEMY supervisor system is used to monitor the system and to edit and store the process recipes.

The THERMCO “6A-CMOS- Poly” horizontal reactor is for CMOS process only.

Safety:

Silane SiH4 is a Pyrophoric gas , extremely flammable when it comes in contact with Oxygen or air. The Material Data Safety Sheet (MSDS) is in the yellow binder. PH3 in 98.5% SiH4 mixture is a dangerous gas too. The system has hardware and software safety interlocks, to prevent any Silane related hazard High temperature: many furnace parts can be hot. Use caution when handling them.

Procedure:
  1. Engage Machine in CORAL for ICL “6A-nPoly” machine, before you start. The wafers should have been RCA cleaned less than 4 hours before and your process must be approved by the PTC.
  2. Pull the tube boat out as follows:
    - On the SEMY terminal double click on “RUN” ; the “Minispec Loader” pops up on the screen.
    - From the OPTION/ TUBE menu choose “6A”
    - Click on File/Open menu , select the “POLY BOAT_OUT” minispec and click OK
    - On Minispec Loader window click “Compile & Send”; Compile Status window will be show up.
    Wait until the OK button is active, then click on it: the recipe was successfully sent to the TMX tube computer
    Note: The tube should be in “Standby” mode to accept a new recipe; if it is in “Complete” status, push the “STOP” button on the tube TMX display to bring the system in ” Standby “ mode. If the tube is in the HOLD mode then push START & STOP buttons in that sequence to bring it in Standby mode.
    - On the tube TMX display push the “START” button; the system will go in Processing mode, and the boat will come out in 30 minutes.
  3. Pull the central quartz boat from the tube paddle using the pick up tool, place it on the designated Poly transfer quartz plate, unload the dummy wafers and place your wafers and Poly monitors with the flat up, in the quartz boat.
    Place the quartz boat back in the central position on the tube paddle, with the wafers front side facing the Source Zone end.
  4. Start the processing recipe, by following these steps:
    - On the SEMY terminal double click on “RUN” icon; the “Minispec Loader” pops up on the screen.
    - From the OPTION/ TUBE menu choose “6A”
    - Click on File/Open menu , select the “625DOPED PH3” minispec and click OK
    - On Minispec Loader window click “Compile & Send; the Compile Status window and the Variable Delay Entry window will show up. On the Variable Delay Entry window input the deposition time and push “ENTER”, input the deposition time again to confirm and wait until the OK button on the Compiler Status window is active, then click on it: the recipe was successfully sent to TMX tube
    computer
    Note: The tube should be in “Standby” mode to accept a new recipe; if it is in “Complete” status, push the “STOP” button on the tube TMX display to bring the system in ” Standby “ mode.
    - On the TMX tube display push “START” button, the system will go in the “Processing” mode.
  5. When the process is finished, take the quartz boat from the tube paddle, using the pick up tool and place it on the designated transfer quartz plate. Remove your process wafers and Poly monitor wafers from the quartz boat and replace them back with the original dummy wafers. Place the quartz boat back on the tube paddle and put the boat in by following these steps:
    - On the SEMY terminal double click on “RUN” icon; the “Minispec Loader” pops up on the screen.
    - From the OPTION/ TUBE menu choose “6A”
    - Click on File/Open menu , select the “POLY BOAT_IN” minispec and click OK
    - On Minispec Loader window click “Compile & Send”: the Compile Status window shows up.
    Wait until the OK button is active, then click on it: the recipe was successfully sent to the TMX tube computer.
    Note: The tube should be in “Standby” mode to accept a new recipe; if it is in “Complete” status, push the “STOP” button on the tube TMX display to bring the system in ” Standby “ mode.
    - On the tube TMX display push the “START” button; the system will go in Processing mode, and the boat will start going in.
“Disengage Machine” in CORAL, after you input the test data from the monitor wafers into the comments section of the engage machine window.
Author: Bernard Alamariu, 1/11