[labnetwork] Carbon contamination from Ar
Mike Young
myoung6 at nd.edu
Sat Oct 28 10:58:05 EDT 2017
Hi Kevin. Have you confirmed the deposits are in fact carbon? Scrape
some off and perfom EDX in a SEM, for example?
--Mike
On 10/28/2017 12:19 AM, Kevin McPeak wrote:
> Dear Colleagues,
>
> In my lab at LSU we are interested in evaporating Au under high Ar
> pressures, 10 - 50 mTorr. We are using Ar 5.0 purity (99.999%), which
> has a THC of 1 ppm.
>
> Our procedure is such:
>
> 1). Pump chamber down to low -7 Torr range
> 2). Inject 30 SCCM Ar and throttle gate valve to the desired pressure
> (say 50 mTorr)
> 3). Increase power to Tungsten boat till Au pellets evaporate
>
> When we vent the chamber_*we notice a lot of carbon deposition*_ near the
> outlet of the Ar line (see attached image). We have a THC of 1 ppm in
> the Ar tank. We also tried hooking up a GP-100 gas purifier from RD
> Mathis. Unfortunately, that didn't solve the problem, still lots of
> carbon deposition in the chamber. The GP-100 is currently connected
> upstream from the MFC. I am using SS tubes with all VCR fittings
> (total length 6 ft). We could move the GP-100 closer to the chamber,
> post-MFC.
>
> Based on the photo I think it is pretty clear that the carbon is
> coming from the Ar. So my current thought is that either I have a leak
> in my tubes post GP-100 or I need to flame bake the lines (I have not
> done this). I am trying to get access to an RGA to investigate this
> more quantitatively. I do have access to a He checker so I could try
> pumping on the Ar lines.
>
> Have any of you seen Carbon contamination like this before when doing
> high-pressure evap (I know that is not a normal thing)? I am curious
> what people think. Thanks!
>
> Regards,
> Kevin
>
--
Michael P. Young (574) 631-3268 (office)
Nanofabrication Specialist (574) 631-4393 (fax)
Department of Electrical Engineering (765) 637-3784 (cell)
University of Notre Dame mike.young at nd.edu
B-38 Stinson-Remick Hall
Notre Dame, IN 46556-5637
-------------- next part --------------
An HTML attachment was scrubbed...
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20171028/ad464dae/attachment.html>
More information about the labnetwork
mailing list