[labnetwork] Lithium evaporation
Morrison, Richard H., Jr
rmorrison at draper.com
Tue Sep 17 05:33:20 EDT 2019
Thanks Clark excellent information.
Rick
From: Clark O.D. [mailto:odc1n08 at soton.ac.uk]
Sent: Tuesday, September 17, 2019 3:43 AM
To: Morrison, Richard H., Jr <rmorrison at draper.com>; labnetwork at mtl.mit.edu
Subject: RE: Lithium evaporation
Can be done and evaporates fairly reliably. It takes very little power to melt. For us it helped to keep the walls of the crucible cold to stop it creeping up the sides and out onto the hearth. Can't remember what crucible we used but a TiN coating is probably not a bad idea to try and stop Li interdiffusion. There is various literature which discusses it being an effective barrier to Li. Pyrolytic Boron Nitride is another good alternative.
It also evaporates well from a k-cell at ~500C but eventually it will creep around the end of your crucible and attack heating filaments if you run it too long. PBN crucibles again.
From: labnetwork-bounces at mtl.mit.edu<mailto:labnetwork-bounces at mtl.mit.edu> <labnetwork-bounces at mtl.mit.edu<mailto:labnetwork-bounces at mtl.mit.edu>> On Behalf Of Morrison, Richard H., Jr
Sent: 13 September 2019 16:55
To: labnetwork at mtl.mit.edu<mailto:labnetwork at mtl.mit.edu>
Subject: [labnetwork] Lithium evaporation
Hi Folks,
Has anybody allowed Lithium into an E-Beam evaporator, if so any tips?
Thanks
Rick
Richard H. Morrison
Principal Member of the Technical Staff
Draper
555 Technology Square
Cambridge, MA
02139-3573
Work 617-258-3420
Cell 508-930-3461
www.draper.com<https://eur03.safelinks.protection.outlook.com/?url=http%3A%2F%2Fwww.draper.com&data=01%7C01%7Codc1n08%40soton.ac.uk%7Cf1928ef3fc9341b524f008d738848f1f%7C4a5378f929f44d3ebe89669d03ada9d8%7C0&sdata=%2FFHH1O3GtSGFcp0rjfUroisuzbOAV2dlDz5WghO3x8k%3D&reserved=0>
________________________________
Notice: This email and any attachments may contain proprietary (Draper non-public) and/or export-controlled information of Draper. If you are not the intended recipient of this email, please immediately notify the sender by replying to this email and immediately destroy all copies of this email.
________________________________
________________________________
Notice: This email and any attachments may contain proprietary (Draper non-public) and/or export-controlled information of Draper. If you are not the intended recipient of this email, please immediately notify the sender by replying to this email and immediately destroy all copies of this email.
________________________________
-------------- next part --------------
An HTML attachment was scrubbed...
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20190917/07433128/attachment.html>
More information about the labnetwork
mailing list