[labnetwork] ZEP worth it?
Lapointe, Jean
Jean.Lapointe at nrc-cnrc.gc.ca
Fri Apr 30 07:08:51 EDT 2021
Hi Long,
It does last for years, about the same as PMMA as far as I can tell. We just finished a bottle with a 2016 expiry and saw no change after opening a new bottle.
It was stored at room T.
It can withstands plasma etching much better than PMMA but doesn’t have as good an adhesion to semiconductors. So it is not a good mask for wet etching semiconductors.
It works very well for lift-off.
It is expensive but can easily be diluted to get thinner films.
It can also be developed in N-amyl acetate; much safer than xylene and with the same contrast and dose-to-clear.
Jean
From: labnetwork [mailto:labnetwork-bounces at mtl.mit.edu] On Behalf Of Chang, Long
Sent: April 29, 2021 10:29 AM
To: labnetwork at mtl.mit.edu
Subject: [labnetwork] ZEP worth it?
***ATTENTION*** This email originated from outside of the NRC. ***ATTENTION*** Ce courriel provient de l'extérieur du CNRC
Hi Guys,
I have no experience with ZEP, but the data sheet suggest a critical dose of ~35 uC/cm2, approximately 1/10 of PMMA. What are the problems with ZEP and under what conditions is it worth the cost? Does it last forever in storage like PMMA?
Thanks,
Long
-------------- next part --------------
An HTML attachment was scrubbed...
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20210430/2989ef18/attachment.html>
More information about the labnetwork
mailing list