Given the size of the defects and the lack of a comet tail in the resist, it looks like small droplets landed on the photoresist film near the end or after the wafer finished spinning.
The droplets could be from aerosolized photoresist/solvent micro droplets generated during spin coating.
Another possibility would be splashed acetone droplets, from wetting a fabwipe in close proximity.
The defects appears to be surface wrinkling whose pattern is the result of stress minimization in the photoresist skin as the extra solvent dries.
Bill
From: labnetwork <labnetwork-bounces at mtl.mit.edu> On Behalf Of Lino Eugene
Sent: Saturday, October 23, 2021 9:28 AM
To: Eva Rose <eva.rose at gno.de>
Cc: labnetwork at mtl.mit.edu
Subject: Re: [labnetwork] Defects after resist spinning
Hi Eva,
It looks like that there is dendritic cristallisation in your defects.
Was the subtrate immersed in RCA 1 or BOE or any solution involving a salt? If so, my first thought is that the substrate was not rinsed properly prior spin coating.
Best,
Lino Eugene
On Oct. 23, 2021 07:46, Aaron Hryciw <ahryciw at ualberta.ca<mailto:ahryciw at ualberta.ca>> wrote:
Hi Eva,
Out of curiosity, did you previously inspect the wafer in an optical microscope using a higher-mag objective than the one used to capture the images? Given how circular these defects look, and the concentric pattern, my guess is that this is a heating effect, the result of staying too long in one position with a high light intensity.
Cheers,
– Aaron
Aaron Hryciw, PhD, PEng
Fabrication Group Manager
University of Alberta - nanoFAB
W1-060 ECERF Building
9107 - 116 Street
Edmonton, Alberta
Canada T6G 2V4 Ph: 780-940-7938
www.nanofab.ualberta.ca<http://www.nanofab.ualberta.ca/>
On Fri, Oct 22, 2021 at 5:55 PM Eva Rose <eva.rose at gno.de<mailto:eva.rose at gno.de>> wrote:
Dear all,
did anybody ever see any defects like this on the resist surface after resist spinning. The diameter varies from about 20um to over 150um.
[cid:17caaeab150a3a20b871]
[cid:17caaeab15074e3f89d2]
Any idea what the reason could be?
Best regards,
Eva
_______________________________________________
labnetwork mailing list
labnetwork at mtl.mit.edu<mailto:labnetwork at mtl.mit.edu>
https://mtl.mit.edu/mailman/listinfo.cgi/labnetwork
________________________________
Notice: This email and any attachments may contain proprietary (Draper non-public) and/or export-controlled information of Draper. If you are not the intended recipient of this email, please immediately notify the sender by replying to this email and immediately destroy all copies of this email.
________________________________
-------------- next part --------------
An HTML attachment was scrubbed...
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20211102/dcb1c0f4/attachment.html>
More information about the labnetwork
mailing list