Hi Ron,
Having a fluorine and chlorine in one system is a controversial issue and some people would love it and others would hate.
Some manufacturers advise to have SF6 along chlorine for a system to etch mainly III-V semiconductors as SF6 is used for cleaning purposes. That said I worked in the past with systems sharing both chemistries. At the moment we have two systems one fluorinated and one chlorinated.
Mixing the gases has pros and cons:
Pros:
1- Economic as 1 system is purchased to etch both III-V and dielectrics/Si. In this case ways to avoid problems is to dedicate a lap of time for Cl-based and another for F-based chemistry with a cleaning in between.
2- Cl2 + SF6 offers the possibility of performing selective etch of GaAs/GaN wrt AlGaAs/AlGaN if required
3- Personally in an RIE system I got4x higher etch rate and smooth when etching GaN in SiCl4+SF6 vs SiCl4 (RIE system and not ICP nor ECR).
Cons:
1- May affect reproducibility, however a good policy for switching the chemistries may address this concern.
2- May not be suitable to achieve best performance in Si etching
Happy to discuss further, if required, off-line any issue.
Best regards,
Fouad Karouta
*************************************
Manager ANFF ACT Node
Australian National Fabrication Facility
Research School of Physics and Engineering
L. Huxley Building (#56), Mills Road, Room 4.02
Australian National University
ACT 2601, Canberra, Australia
Tel: + 61 2 6125 7174
Mob: + 61 451 046 412
Email: fouad.karouta at anu.edu.au<mailto:fouad.karouta at anu.edu.au>
http://anff-act.anu.edu.au/
From: labnetwork-bounces at mtl.mit.edu [mailto:labnetwork-bounces at mtl.mit.edu] On Behalf Of McWilliams, Scott
Sent: Friday, 9 November 2018 12:17 PM
To: James P McVittie <mcvittie at stanford.edu>; Reger, Ronald K <rreger at purdue.edu>; labnetwork at mtl.mit.edu
Subject: Re: [labnetwork] Mixing Fluorine and Chlorine Chemistries
Ron,
I believe in your case, you are more concerned about switching from one application to another and not so concerned about sequentially using fluorine and chlorine in the same application, right? In addition to Jim's comments about removing oxides in Poly Si etching, when I worked at Lam Research, the gate-level polysilicon etch tools used HBr and chlorine chemistries and the chamber cleans in the same chamber always used fluorine-based gases such as NF3. The protocol for going from one application to another was a fluorine based chamber clean followed by the cycling of application specific dummy wafers. I am unaware of any failure physics/mechanisms of using both chemistries and it will be interesting to hear others respond to this.
Also, as Jim pointed out, for III/V processing, many fabs use chlorine/methane/hydrogen type processes that form polymers on just about everything in the chamber, including the mask on the wafer. My own data for low volume III/V processing showed that when I used fluorine based chemistry to open dielectric masks, followed by a chlorine-based ICP etch to etch III/V compounds, we had issues with etch rate and profile control (I should have talked to Jim before trying this!).
Regards, Scott
From: labnetwork-bounces at mtl.mit.edu<mailto:labnetwork-bounces at mtl.mit.edu> [mailto:labnetwork-bounces at mtl.mit.edu] On Behalf Of James P McVittie
Sent: Thursday, November 08, 2018 5:58 PM
To: Reger, Ronald K <rreger at purdue.edu<mailto:rreger at purdue.edu>>; labnetwork at mtl.mit.edu<mailto:labnetwork at mtl.mit.edu>
Subject: Re: [labnetwork] Mixing Fluorine and Chlorine Chemistries
Ron,
1. F in an etch chamber from previous etch runs can slow down a Cl2 etching process. This is of most concern to III-V users. So for a well-controlled Cl2 etch process you want to get all the F based polymers out of the chamber.
2. In Poly Si etching C2F6, CF4 or NF3 are often used to remove surface oxides before start the HBr / Cl2 Si etch.
3. " Small amounts of CF4 (5-10 sccm) are added to the standard BCl3/Cl2/N2 process for residue removal. In some cases (particularly for copper residue), CF4 appears to widen the process window for residue control.CF4 typically helps to eliminate open field residue, but there have been cases where CF4 helped with dense area residue as well. Since the addition of another gas introduces more variables to the process, the use ofCF4 should be minimized." From old AMT Metal (Al) Etch Process Manual
In the Stanford Nanofabrication Facility (SNF) we have F containing gases in all our Cl2 etchers. Our Cl2 Si etchers have CF4 and C2F6. Our ICP metal etcher has CF4, and Our III-V etcher has SF6.
James (Jim) McVittie, Ph.D.
Senior Research Engineer
Electrical Engineering
Stanford University
336x Paul G. Allen Bldg
420 Via Palou Mall
Stanford, CA 94305
mcvittie at stanford.edu<mailto:mcvittie at stanford.edu>
650-725-3640
________________________________
From: labnetwork-bounces at mtl.mit.edu<mailto:labnetwork-bounces at mtl.mit.edu> <labnetwork-bounces at mtl.mit.edu<mailto:labnetwork-bounces at mtl.mit.edu>> on behalf of Reger, Ronald K <rreger at purdue.edu<mailto:rreger at purdue.edu>>
Sent: Thursday, November 8, 2018 10:45 AM
To: labnetwork at mtl.mit.edu<mailto:labnetwork at mtl.mit.edu>
Subject: [labnetwork] Mixing Fluorine and Chlorine Chemistries
Dear Colleagues,
Here at the Birck Nanotechnology Center we have a Panasonic E620 RIE ICP etcher that uses a variety of gases for etching of various materials. It has capability to do both chlorine-based and fluorine-based processes. This has given us a lot of versatility for a wide variety of materials. We're now exploring the implications of using both chemistries in the same etcher, particularly when it comes to making electron devices.
We had done a small survey of a few other facilities and are finding a mixed response..... some facilities use dedicated etchers to keep these chemistries separated while others have both gases in the same etcher and use one type of recipe or the other. Particularly for electron devices are there cross-contamination issues/models with using both gases in the same chamber? What would be the failure physics/mechanisms from this? If both chemistries are used in the same system are there standard protocols between switching etch chemistries that we need to follow?
Any advice would be greatly appreciated as we're getting into more electron device processing!
Thanks,
Ron
Ron Reger
Engineering Manager
Birck Nanotechnology Center | Room 2289 |
Office: 765.494.6667 | Email: rreger at purdue.edu<mailto:rreger at purdue.edu>
Wiki: https://wiki.itap.purdue.edu/display/BNCWiki
iLabs: https://purdue.ilabsolutions.com/homepage/
______________________________________________________________
[Purdue_University-150_Years_of_Giant_Leaps.png (300?-66)]
www.purdue.edu/giantleaps<http://www.purdue.edu/giantleaps>
-------------- next part --------------
An HTML attachment was scrubbed...
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20181112/303a3444/attachment.html>
-------------- next part --------------
A non-text attachment was scrubbed...
Name: image001.png
Type: image/png
Size: 11196 bytes
Desc: image001.png
URL: <https://mtl.mit.edu/pipermail/labnetwork/attachments/20181112/303a3444/attachment.png>
More information about the labnetwork
mailing list